1. Home
  2. Resources
  3. Surface before bonding

Technical article, adhesion

Surface Preparation Before Bonding: Measuring Surface Energy and Validating Adhesion

The short answer

Before bonding, you check that the surface has enough energy for the adhesive to spread on it. In practice, the aim is 40 to 44 mN/m for bonding and laminating, and 38 mN/m for printing; the exact threshold depends on your adhesive or ink. You measure it with a test ink, in seconds on the line, then validate adhesion with the real adhesive. If the surface is too low, an atmospheric plasma treatment raises it just before bonding, dry and with no solvent. Kalego Solutions, from Quebec City (Canada), runs this test on your parts.

Have my parts tested

Updated November 5, 2026 by the Kalego Solutions team, Quebec City (Canada)

40 to 44 mN/m

Usual threshold for bonding

38 mN/m

Usual threshold for printing

Test ink

Measured in seconds

0 solvent

Atmospheric plasma, dry

Surface before bonding

  • Measure
  • The thresholds
  • Why it fails
  • Validate
  • Questions

Measuring surface energy before bonding

Surface energy tells you whether a liquid will spread on the part or bead up. An adhesive whose surface tension is higher than the part's does not spread and does not form a strong bond.

A calibrated test ink is applied with a brush or a pen: it spreads if the surface is above the ink value, and beads up below it. The measurement takes seconds and can be done on the line.

Which value to aim for

UseTarget surface energy
Printing38 mN/m
Bonding and laminating40 to 44 mN/m
Usual industry values. The exact threshold depends on your adhesive or ink, and is confirmed by a test.

Why the adhesive does not hold

A low surface energy material

Untreated polypropylene is around 30 mN/m and polyethylene around 31.6 mN/m: below the bonding threshold.

Contamination

Release agent, oil or dust prevent contact. Plasma removes a thin organic contamination layer, not a thick film: a prior degreasing step is then still needed.

An activation that has faded

The effect of a treatment decays with time. Bonding must follow the treatment closely enough.

Validating adhesion in three tests

  1. Measure the surface

    Surface energy with test ink, or contact angle, before and after treatment.

  2. Test adhesion

    With your real adhesive: peel test, or cross-cut test per ISO 2409 for a paint.

  3. Check over time

    Repeat the measurement after the real delay between treatment and bonding on your line.

Have our lab run these tests →

Frequently asked questions about preparation before bonding

What surface energy is needed for bonding?

In practice, the aim is 40 to 44 mN/m for bonding and laminating, and 38 mN/m for printing. The exact threshold depends on your adhesive or ink.

How do you measure surface energy?

With a calibrated test ink, in seconds on the line, or by contact angle measurement in a lab.

Does plasma replace a primer?

Often, but not always. It replaces the adhesion step when the adhesive bonds on the activated surface; a test on your material and adhesive pair confirms it.

How long between treatment and bonding?

As little as possible: the effect decays with time. We measure the real window on your part.

Does plasma also clean the part?

It removes thin organic contamination, not a thick film of release agent or oil. A prior degreasing step is then still needed.

Where is Kalego Solutions located?

In Quebec City, Canada. The company designs, builds and tests its equipment there, since its founding at Université Laval in 2019.

Kalego Solutions at a glance

Kalego Solutions designs and manufactures atmospheric plasma (DBD) surface treatment equipment in Quebec City, Canada. It integrates into production lines with no vacuum chamber and no chemical solvents. Spun out of Université Laval research, the company serves manufacturers in Canada and the United States.

Headquarters and lab
Quebec City (QC), Canada
Technology
Atmospheric-pressure DBD plasma, no vacuum
Manufacturing
Designed, built and tested in Quebec City
Origin
Université Laval, founded December 2019, incorporated 2022
Partners
Université Laval, CHU de Québec, NRC, Mitacs, ACXYS
Markets served
Canada and the United States
Contact
[email protected], reply within 48 business hours

Sources

  1. Accu Dyne Test, critical surface tension of polymers
  2. Šrámková et al., Polymers 13, 4173 (2021)
  3. Leroux et al., Journal of Colloid and Interface Science 328, 412 (2008)
  4. Shaw et al., Plasma Sources Science and Technology 25, 065018 (2016)
  5. 3M, categorizing surface energy
  6. ISO 2409, cross-cut test for paints and varnishes
  7. Kalego Solutions, surface energy test inks
  8. Kalego Solutions, adhesion application

Our work is covered by

  • Radio-Canada
  • Les Affaires
  • Design Engineering
  • Innovation News Network
  • Mitacs
  • Acfas

Let's check your parts before bonding.

Request a trial See the test inks
10, rue de l'Espinay, E0170
Quebec City, QC G1L 3L5, Canada
[email protected]